Self-Leveling Compound Additives: Flow, Stability and Crack Resistance

Flow, bleed control and strength for cement- and gypsum-based floor levelers.

LANDU: Your Self-Leveling Compound Additives Manufacturer

A self-leveling compound has to flow like a liquid for 20–30 minutes, then behave like a strong, crack-free screed for 20 years. Those two demands pull in opposite directions, and the additive package is what reconciles them: a superplasticizer for flow at low water, a very low-viscosity cellulose ether to keep sand and water together, a polymer powder for flexibility and surface strength, and a defoamer to release the air that pumping puts in. Below are the Landercoll®, Accurate® and NOVASTAR® grades we recommend for each system, with starting dosages and a troubleshooting table.

What EN 13813 and the job site expect

PropertyHow it is judgedTypical targetControlling additive
FlowRing test (e.g. Ø 30 × 50 mm ring)130–150 mm spread, loss ≤ 10 mm after 20 minPCE type and dosage, cellulose ether viscosity
Bleeding / segregationVisual, after 10 min at restNo water film, no sand settlementLow-viscosity HPMC, defoamer compatibility
SurfaceVisual after 24 hNo pinholes, craters or laitancePowder defoamer, water content
Strength classEN 13892-2CT-C25-F6 to CT-C35-F7 (cement); CA-C20-F4 to CA-C30-F6 (gypsum)Water/binder ratio set by PCE; RDP for flexural strength
Walkability / overlaySite scheduleWalkable 3–4 h, tiles after 24 h, resilient flooring 48–72 hBinder system (OPC/CAC/CSA), accelerator, PCE profile
Dimensional stabilityShrinkage prism, visualNo curling, no crackingRDP, water reduction, shrinkage control
Wear resistanceEN 13892-3/4 (A/AR classes)Declared when used as wearing layerRDP dosage, low w/b

Grade selection by system

SystemLandercoll® cellulose etherAccurate® RDPNOVASTAR® PCENOVASTAR® defoamerOther
Cement-based underlayment (OPC + CAC + anhydrite/gypsum)K04 (300–500 mPa·s) 0.03–0.06 %Rigid 5011N 1.5–3 % or semi-flexible 4025N 2–3 %540P or 550P, or TDS-series 590P, 0.15–0.35 %P805, 0.1–0.3 %Tartaric acid / Li₂CO₃ for set control
Cement-based wearing layer, high strengthK04 0.03–0.05 %4025N or 5045N, 3–4 %540P / 550P or 590P, 0.2–0.4 %P805, 0.15–0.3 %PP fibre 6 mm 0.05–0.1 %
Gypsum-based (α-hemihydrate or anhydrite)K04 0.03–0.06 %4025N or 5045N, 1–2 %570P (gypsum system) or 590P, 0.1–0.3 %P805, 0.1–0.2 %Gypsum retarder P400 / AR-P, 0.02–0.05 %
Rapid-setting CAC-rich repair levelerK04 0.02–0.04 %5011N, 1–2 %590FP (early strength), 0.15–0.3 %P805 (P807 in cold weather), 0.1–0.2 %Lithium carbonate accelerator
Pumpable large-area flooringK04 0.03–0.06 %5011N or 4025N, 2–3 %550P, or 590P + 600P (slump retention), 0.2–0.4 % totalP805 (P806 alkali-resistant on request), 0.15–0.3 %—
Waterproof / wet-room levelerK04 0.03–0.05 %8048H (TDS lists cement-based self-leveling mortar), 2–3 %540P or 590P, 0.15–0.3 %P805, 0.15–0.3 %—

Dosages are percentages of the total dry mix for laboratory starting points; the technical data sheets do not prescribe dosages. Cellulose ether in self-leveling compounds is dosed ten times lower than in tile adhesive; 0.01 % steps matter. The PCE technical data sheets give 0.1–0.5 % of cementitious material as the recommended range — the mortar-based figures above fall inside it once converted.

Why these grades:

  • K04 is the low-viscosity Landercoll® HPMC made for flooring: 300–500 mPa·s (Brookfield RV and NDJ-1, 2 %), final consistency “very low”, and the TDS lists “increased leveling, surface aesthetics” and “improved flexural and tensile bond strength” among its properties. It suppresses bleeding and sand settlement without pulling flow down; a 0.02 % overdose costs 10–15 mm of spread, so viscosity, not dosage, is the main lever. See HPMC viscosity for self-leveling mortar.
  • Accurate® 5011N (rigid, Tg 10 ± 5 °C) is the economical choice for underlayments that will be covered; 4025N (semi-flexible, Tg 0 °C) and 5045N (flexible, Tg −10 ± 5 °C) add flexural strength, abrasion resistance and surface quality to wearing layers; 8048H is the instant-dissolving, very strongly hydrophobic grade whose TDS lists cement-based self-leveling mortar.
  • NOVASTAR® PCE 530P–580P series: 540P (sulfoaluminate-cement water reducer, water-reduction rate 34 % on the product page) and 550P are the recommended grades for cement-based self-leveling; 570P (gypsum system, 37 %) is the recommended grade for gypsum-based self-leveling; 580P (37 %) is compatible with both.
  • NOVASTAR® PCE 590P (TDS series) is the high-water-reduction powder polycarboxylate (water-reduction rate ≥ 25 %, 97 % solids, moisture ≤ 3 %, chloride ≤ 0.02 %, alkali ≤ 2.0 % Na₂O eq., heat-resistant to 50 °C). 600P has the same specification with a long-lasting slump-retention profile for pumped and large-area work; 590FP adds early-strength functional groups (compressive strength ratio > 240 % at 12 h and ≥ 200 % at 1 day in the TDS test, setting shortened by more than an hour) for rapid-set levelers. None of them may be combined with naphthalene sulfonate superplasticizers.
  • P805 / P806 / P807 are the NOVASTAR® powder defoamers: P805 is the standard grade, P806 the alkali-resistant version for high-pH, cement-rich binders, P807 the low-temperature version for winter production and cold-climate sites.

Troubleshooting: what the surface tells you

SymptomLikely causeAdjustment
Water film and sand at the bottom after 10 minCellulose ether too low or absent; too much waterAdd 0.01–0.02 % K04; cut water 0.5 %; check PCE overdose
Spread falls from 145 to 120 mm in 15 minCement–PCE incompatibility, high temperature, C₃A-rich cementReplace part of the 590P with 600P (slump retention); test with the second cement source
Pinholes and cratersAir from mixing/pumping not released; wrong defoamer typeRaise P805 to 0.2–0.3 % or move to P806 in cement-rich mixes; check K04 dosage
Random cracking after 1–3 daysHigh water, fast drying, no polymerLower w/b via PCE; 2–3 % RDP; protect from draughts for 24 h
Curling at edgesDifferential drying, low polymer3 % 4025N or 5045N; reduce layer thickness variation; cure
Dusting, weak surfaceBleeding carried fines up; low RDPFix bleeding first (K04), then RDP ≥ 2 %
Too sticky, poor self-healing of trowel marksCellulose ether viscosity too high (a K40 or higher grade instead of K04)Use K04 only
Slow strength gain in gypsum SLCOver-retarded; PCE overdosedReduce retarder to 0.02 %; keep 590P ≤ 0.3 % and verify with the actual gypsum source
Walk-on time too long in a repair levelerBinder too slow for the schedule590FP (early-strength PCE) with lithium carbonate; check CAC share

Detailed case studies: Preventing cracking in self-leveling compounds · Cracks after curing · Bleeding and segregation.

Starting formulation (cement-based underlayment, dry mix)

ComponentShare
CEM I 52.5 R25 %
Calcium aluminate cement10 %
Anhydrite or α-gypsum5 %
Quartz sand 0.1–0.6 mm50 %
Limestone filler9 %
Landercoll® HPMC K040.04 %
Accurate® RDP 4025N2.5 %
NOVASTAR® PCE 590P0.25 %
NOVASTAR® defoamer P8050.2 %
Tartaric acid / lithium carbonate0.05–0.15 % (set control)
Water≈ 20–22 % of dry mix

Laboratory starting point only; the ternary binder ratio and set control must be tuned to local cement and the required walk-on time.

Products referenced on this page

Why flooring producers work with LANDU

Self-leveling compounds expose weak additives faster than any other product: a batch of cellulose ether 20 % off viscosity shows up as bleeding on the next job. LANDU controls viscosity batch by batch in its own plants (three production bases, 75,000 t/year), supplies REACH-compliant grades under ISO 9001, and runs flow, bleeding and strength tests on customer formulations in its Jinan application laboratory. European customers are served through partners in several countries, including Greece, Spain and Italy, with 25 kg bags on pallets and 7–15 working-day factory lead times. Shelf life per TDS: K04 two years, RDP one year (use within six months of receipt recommended), PCE powder twelve months in the original packaging.

Self-Leveling Compound Additives: Frequently Asked Questions

Answers on additive selection, testing, samples and supplier qualification.

Which HPMC viscosity should be used in a self-leveling compound?

300–500 mPa·s (Landercoll® K04, the only Landercoll® grade whose TDS is written for self-leveling compounds) at 0.02–0.06 %. Tile-adhesive and putty grades (K40 and above, 18,000 mPa·s and higher) destroy flow and should not be used.

How much PCE does a dry-mix self-leveling compound need?

Typically 0.15–0.35 % of the dry mix for NOVASTAR® 540P / 550P or the TDS-series 590P, which corresponds to the 0.1–0.5 % of cementitious material given on the TDS. Start at 0.25 %, measure spread at 0 and 20 minutes, and adjust in 0.05 % steps. Overdosing shows up as bleeding and retarded setting.

Do I need RDP in an underlayment that will be covered by tiles?

Yes, at 1.5–3 %. Even under tiles, the polymer film gives the tensile and flexural strength that stops cracking and curling and secures the bond to the tile adhesive above it. 5011N is the economical rigid grade; 4025N adds flexibility.

Which defoamer grade: P805, P806 or P807?

Start with P805, the standard grade, at 0.1–0.3 %. P806 is the alkali-resistant version for cement-rich, high-pH binders where standard defoamers lose activity; P807 is the low-temperature version for winter production and cold sites. Our technical team sends a comparison sample for your binder.

What changes for a gypsum-based self-leveling compound?

Keep K04 at 0.03–0.06 %, use the gypsum-system PCE 570P (or 590P) at 0.1–0.3 % and confirm its water reduction on your calcium sulphate binder, add 0.02–0.05 % gypsum retarder (P400 or the alkali-resistant AR-P) for working time, and use 1–2 % semi-flexible 4025N or flexible 5045N.

Can LANDU test my formulation?

Yes. Send 5 kg of your dry mix or the recipe; our laboratory reports spread at 0/10/20 min, bleeding, setting time, 1-, 7- and 28-day strength and surface appearance, with recommended adjustments.

What does HPMC do in self-leveling mortar?

At 0.03–0.06 % a very low-viscosity grade (Landercoll® K04, 300–500 mPa·s) holds water and fines together so the mix flows as one liquid instead of separating into a water film on top and sand at the bottom. It is a stabiliser, not a thickener: any grade above K04 makes the compound sticky and stops trowel marks from healing. Flow comes from the PCE; the HPMC only has to be enough to stop bleeding and settlement.

Do you manufacture HPMC for self-leveling mortar, and can we buy in bulk?

Yes. Landercoll® K04 is made in LANDU's own cellulose ether plants in Shandong, as are the NOVASTAR® PCE and defoamer and the Accurate® RDP on this page. Minimum order 1,000 kg per grade in 25 kg bags on 500 or 600 kg pallets; stock grades ship in 7–14 days, FOB or CFR/CIF to European ports. A 500 g – 1 kg sample with TDS and batch COA is free.

Why is my self-leveling underlayment cracking?

Cracks in the first 1–3 days are drying shrinkage: too much water, too fast drying, or too little polymer. Bring the water down with PCE rather than by cutting flow, add 2–3 % RDP (4025N or 5045N), and keep the floor out of draughts and direct sun for 24 hours. Cracks that follow substrate joints or sit over hollow-sounding areas are substrate problems, not additive problems. Case studies: preventing cracking in self-leveling compounds · cracks after curing.

Request Samples and a Grade Recommendation

Send your current recipe and flow/strength targets.

We return a grade recommendation and dosage plan within two working days and ship samples of K04, 4025N, 590P and P805 free of charge.

LANDU Company

Ask a Formulation Engineer

LANDU — Committed to Every Gram.