Grout is the one mortar that must flow into a space it cannot be pushed into — under a machine base plate, around an anchor bar, into a 3 mm tile joint — and then stay there without bleeding, shrinking or cracking. That behaviour comes from a tightly balanced additive package: a superplasticizer for flow at low water, a trace of cellulose ether to keep the mix cohesive, a defoamer to release pumped-in air, polymer for bond and ductility, and an expansion component for volume stability. This page gives the NOVASTAR®, Landercoll® and Accurate® grades for each grout type, with starting dosages and a troubleshooting table.
| Grout type | Where used | Reference requirements | Additive priorities |
|---|---|---|---|
| Non-shrink precision grout | Machine bases, bearing plates, column bases, precast joints | National specs / EN 1504-6 anchoring: flow 250–300 mm (cone), 1-d strength ≥ 20 MPa, 28-d ≥ 60 MPa, expansion 0–0.3 % at 24 h, no bleeding | High water reduction, bleed control, controlled plastic expansion, air control |
| Pumpable / injection grout | Post-tensioning ducts, voids, masonry consolidation | Marsh-cone flow 20–30 s, bleeding < 0.3 %, volume change ≤ +0.1 / −0.1 % | Flow retention over 60–90 min, anti-washout cohesion, zero bleeding |
| Anchoring grout | Rebar, bolts and rock bolts in drilled holes | EN 1504-6: pull-out displacement ≤ 0.6 mm at 75 kN; early strength | Thixotropy for overhead holes, fast strength, low shrinkage |
| Tile joint grout | Ceramic and stone joints 2–15 mm | EN 13888: CG1 / CG2 (W = reduced water absorption, A = high abrasion resistance) | Workability and clean-off, flexibility, water repellency, colour stability |
| Additive | Grades (TDS data) | Non-shrink precision grout | Pumpable / injection grout | Anchoring grout | Tile joint grout (CG2 WA) |
|---|---|---|---|---|---|
| NOVASTAR® PCE, 530P–580P series (product-page data) | 530P (Portland-cement system, water-reduction rate 34 %) and 550P are recommended for grouting and injection mortar; 540P (sulfoaluminate cement, 34 %) is compatible and suits rapid-setting and pressure grouts; 580P (37 %) is designed for high-strength non-shrink, sleeve and wind-turbine grouts | 530P or 580P 0.3–0.6 % | 530P + 550P 0.3–0.5 % | 540P or 580P 0.2–0.4 % | — |
| NOVASTAR® PCE superplasticizer (TDS series) | 590P — high water reduction (≥ 25 %, 97 % solids, chloride ≤ 0.02 %); 600P — long-lasting slump retention; 590FP — early strength (12 h strength ratio > 240 %, setting shortened > 1 h). TDS dosage 0.1–0.5 % of cementitious material | 590P 0.3–0.6 % of dry mix | 590P + 600P 0.3–0.5 % (600P share rises with placement time) | 590FP 0.2–0.4 % | — or 590P 0.05–0.1 % |
| NOVASTAR® powder defoamer | P805 standard; P806 alkali-resistant; P807 low-temperature | P805 / P806 0.1–0.3 % | 0.1–0.2 % | 0.1–0.2 % | 0.05–0.1 % |
| Landercoll® cellulose ether | K04 (300–500 mPa·s; self-leveling grade), K40 (18,000–20,000 mPa·s; TDS: crack filler / tile grout, masonry mortar), MPE4090-T (35,000–45,000 mPa·s; TDS: crack filler / tile grout, tile adhesive), EM40HT (18,000–23,000 mPa·s; TDS: repair mortar, tile adhesive) | K04 0.02–0.04 % (cohesion without flow loss) | K04 / K40 0.03–0.06 % (anti-washout) | EM40HT 0.10–0.20 % (thixotropy, excellent water retention) | K40 or MPE4090-T 0.15–0.30 % |
| Accurate® RDP | 4012N, 5011N rigid (Tg 10 ± 5 °C); 4025N semi-flexible (Tg 0 °C); 5045N flexible (Tg −10 ± 5 °C); 8032H medium hydrophobic, 8035H strong hydrophobic (TDS: tile grouts); 9028E / 9055E acrylic–silane (TDS: cement-based grouts, anti-soiling) | 5011N 1–2 % (bond, ductility) | — or 5011N 1 % | 4012N / 5011N 1–2 % | 5045N or 4025N 2–4 % + 8035H / 9055E for W class |
| NOVASTAR® SHP hydrophobic powder | SHP75 / SHP80 (TDS: grouts and joint fillers; dosage 0.1–0.5 %) | — | — | — | 0.2–0.5 % (W class, stain resistance) |
| NOVASTAR® starch ether | ST3152 (machine-applied mortars, thixotropy), ST3547 (universal, low ash) | — | — | ST3152 0.02–0.05 % (overhead holes) | ST3547 0.02–0.05 % (creamy clean-off) |
| PP fibre | 3–6 mm | 0.05–0.1 % | — | 0.05–0.1 % | — |
| Expansion component (third-party) | Plastic-phase (Al-powder based) and/or hardened-phase (CSA / CaO) expansive agent | as required for 0–0.3 % | as required | as required | — |
Dosages are percentages of the total dry mix for laboratory starting points; the technical data sheets do not prescribe mortar dosages. In high-flow grouts cellulose ether is dosed in hundredths of a percent; use K04 and adjust in 0.005 % steps. PCE powders must not be combined with naphthalene sulfonate superplasticizers, and compatibility with other admixtures has to be tested (TDS).
| Symptom | Likely cause | Adjustment |
|---|---|---|
| Water film on top after 15 min (bleeding) | No cohesion component; PCE overdosed | Add 0.01–0.02 % K04; cut 590P by 0.05 %; check sand fines |
| Flow drops from 280 to 220 mm within 30 min | Cement–PCE incompatibility; heat; C₃A-rich cement | Replace part of 590P with 600P (slump retention); cool water; test second cement |
| Pinholes and foam on surface, low density | Entrained air not released | P805 0.2–0.3 % (P806 in cement-rich, high-pH grouts); slower mixing |
| Shrinkage cracks after demoulding | No expansion component; high water | Plastic-phase expander; lower w/b with 590P; cure 3 days wet |
| Grout expands too much, cracks the edge | Over-dosed expander, high temperature | Reduce expander; test expansion at site temperature |
| Pump line blocks, surging | Segregation under pressure; air | K04 0.03 %; P805; constant water dosing; avoid sand > 2 mm |
| Low 1-day strength | High w/b; retardation from overdosed PCE or cellulose ether | 590FP (early-strength PCE) at correct dose; K04 only; P807 and warm water if cold |
| Tile grout cracks or shrinks in wide joints | Low polymer, fast drying | 5045N 3 %; MPE4090-T 0.2 %; fine sand 0–0.5 mm; wet cure |
| Tile grout stains, absorbs water | No hydrophobic component | SHP 0.3 %; hydrophobic RDP 8035H or acrylic–silane 9055E (TDS: lotus effect, anti-soiling) |
| Patchy colour in pigmented grout | Efflorescence and uneven water | SHP; consistent water dosing; low-alkali white cement |
| Component | Non-shrink precision grout | CG2 WA tile grout |
|---|---|---|
| CEM I 52.5 R | 40–45 % | White cement 42.5: 30–35 % |
| Silica fume / fly ash | 3–5 % | — |
| Quartz sand 0–2 mm (grout) / 0–0.3 mm (tile grout) | 48–52 % | 55–60 % |
| Limestone filler | — | 5–8 % |
| NOVASTAR® PCE | 530P or 590P 0.4 % | 590P 0.05 % |
| NOVASTAR® defoamer P805 | 0.2 % | 0.05 % |
| Landercoll® cellulose ether | K04 0.03 % | MPE4090-T 0.20 % |
| Accurate® RDP | 5011N 1.5 % | 5045N 3 % |
| NOVASTAR® SHP75 / SHP80 | — | 0.3 % |
| Expansive agent (plastic-phase) | 0.01–0.03 % Al-based or per supplier | — |
| PP fibre 6 mm | 0.05 % | — |
| Pigment | — | as required |
Starting points only; expansion and early strength must be verified at the temperatures the grout will be placed at.
Grout formulations run at very low cellulose ether and very high superplasticizer dosages, so both must be consistent lot to lot. LANDU manufactures Landercoll® cellulose ethers, Accurate® RDP and NOVASTAR® PCE and defoamers in its own plants in Shandong (three production bases, 75,000 t/year) under ISO 9001, supplies REACH-compliant grades to more than 60 countries and holds European stock with partners in several countries, including Greece, Spain and Italy. Factory lead time 7–15 working days. Packaging per TDS: PCE powder in 25 kg woven bags with PE liner (shelf life 12 months, use within 60 days of opening); cellulose ether and RDP in 25 kg bags on pallets.
NOVASTAR® 530P (Portland-cement system, recommended for grouting) or 580P for high-strength non-shrink and sleeve grouts, at 0.3–0.6 % of the dry mix. From the TDS series, 590P is the high-water-reduction powder polycarboxylate (water-reduction rate ≥ 25 %, 97 % solids, fully water-soluble) at the same dosage. For placement windows beyond 45 minutes blend in 600P, the slump-retention grade; for anchoring and precast grouts that need very high early strength use 590FP, whose TDS reports a 12-hour compressive strength ratio above 240 %.
Only a trace — 0.02–0.04 % of the low-viscosity Landercoll® K04 (300–500 mPa·s). It gives the mix enough cohesion to stop bleeding and segregation under pressure without taking flow away. Tile-adhesive viscosities would turn the grout into a paste.
Three small moves in order: 0.01–0.02 % K04, 0.05 % less PCE, and 0.1–0.2 % P805 defoamer so that air is not mistaken for water on the surface. Check that the sand has 3–5 % fines below 0.1 mm.
Volume stability comes from a plastic-phase expansive agent (aluminium powder-based) or a hardened-phase agent (CSA/CaO type), which are not LANDU products. Our contribution is the low water demand (PCE), bleed control (K04), dense matrix (defoamer) and ductility (RDP) that make the expansion predictable and the hardened grout crack-free.
Landercoll® K40 or MPE4090-T — the grades whose TDS list crack filler / tile grout — at 0.15–0.30 % for clean workability, Accurate® 5045N at 2–4 % for the abrasion and flexibility of class A, and 0.2–0.5 % NOVASTAR® SHP (optionally with the strongly hydrophobic 8035H or the acrylic–silane 9055E) for the reduced water absorption and stain resistance of class W.
Yes. Our laboratory reports flow cone / flow table at 0, 30 and 60 minutes, bleeding, plastic expansion at 3 and 24 hours, air content and 1-, 3- and 28-day strength on your dry mix, with additive adjustments.
The core additive is a PCE superplasticizer (NOVASTAR® 590P, 600P for slump retention or 590FP for early strength, 0.1–0.5 % of cement) for flow at a water/cement ratio low enough for strength and volume stability. Around it: a powder defoamer (P805 or P806, 0.1–0.3 %) to release pumped-in air, a trace of cellulose ether (K04, 0.02–0.04 %) to stop bleeding, an expansive agent for the non-shrink property, and, in tile grout or anchoring grout, RDP or starch ether for adhesion and thixotropy.
Buyers use both words for the same materials. "Admixture" comes from concrete practice, where the chemical is dosed at the mixer; "additive" is the dry-mix term for a powder blended into the bag at the factory. Everything on this page is a factory-blended powder, so we say additives. Selection and testing are the same either way.
When fresh density or air content shows entrapped air, or hardened sections show pores. In pumped or heavily superplasticised grout that is almost always, which is why P805 appears in every column of the selection table. Check the defoamer's effect on flow and bleeding, and do not expect it to fill voids caused by incomplete filling, bleed channels or poor curing.
We return a PCE, defoamer, cellulose ether and polymer recommendation within two working days and ship samples free of charge.