title: "Skim Coat & Wall Putty Additives: HPMC, RDP, HPS"
url: https://landuchina.eu/skim-coat-wall-putty-additives/
description: "Additives for cement, gypsum and exterior wall putty: Landercoll® HPMC/MHEC, Accurate® RDP and starch ether, with dosages against powdering, cracks and sagging."
author: "landuexpand@gmail.com"
date_published: 2026-05-18T09:29:17+00:00
date_modified: 2026-11-09T08:42:58+00:00
language: en-US
type: page
generator: LemonX AEO 1.4.8
---

# Skim Coat & Wall Putty Additives: HPMC, RDP, HPS

Skim Coat & Wall Putty Additives: Smooth Finish Without Powdering or Cracking

Divider

Grades and starting dosages for cement-based, gypsum-based and exterior wall putty.

HPMC for Skim Coat & Wall Putty

Improve water retention, smooth application and open time for better finishing performance.

RDP for Skim Coat & Wall Putty

Enhance adhesion, flexibility and crack resistance in cement-based wall formulations.

HPS for Skim Coat & Wall Putty

Improve anti-sagging performance and application consistency for smoother construction.

LANDU: Your Skim Coat & Wall Putty Additives Manufacturer

Divider

Wall putty is applied in layers of 1–3 mm, so it dries faster and is judged more harshly than any other mortar: powdering, hairline cracks and trowel drag are visible the next morning. The fix is almost never more cement — it is the right cellulose ether grade for the layer thickness, enough polymer to bind the surface, and a starch ether to make the putty move under the blade. This page gives the grades and starting dosages for cement-based, gypsum-based and exterior putties.

Three putty systems, three different additive briefs

Divider

| System | Binder | Where it is used | What the additive package must do | Reference standard |
| --- | --- | --- | --- | --- |
| Cement-based skim coat / exterior putty | White or grey cement + limestone filler | Exterior façades, wet rooms, concrete leveling before paint | Water retention on absorbent substrates, adhesion to concrete and AAC, water resistance, crack control | EN 998-1 (OC/GP render types) |
| Gypsum-based finishing putty | Gypsum hemihydrate (± lime) | Interior walls and ceilings, plasterboard joints and skim | Open time control, sandability, no shrinkage cracking, smooth white surface | EN 13279-1 (C6 thin-coat, C7 finishing plaster) |
| Polymer-modified interior putty | Cement or gypsum with 3–8 % RDP | High-end interior finishing, machine-applied skim | Zero powdering, flexibility over joints, fine texture | EN 998-1 / EN 13279-1 as applicable |

Grade selection

Divider

**Landercoll® cellulose ether.** The technical data sheets list "skim coat / wall putty (powder form)" for K75, K100, EM60, EM80 and EM100, "skim coat / wall putty" for K150, K200, K200H and EM200, and "wall putty / skim coat" for EM100H. For ready-mixed paste putty the TDS recommends the surface-treated, delayed-solubility grades K40HS and K75HS ("latex-based and paste application, wall putties, joint fillers"). For gypsum putty the dedicated HEMC grades are ME3570-G and ME4080-G ("gypsum-based wall putty / skim coat"). Viscosities are Brookfield RV, 2 % solution, 20 °C.

| Putty type | Cellulose ether (viscosity) | Starting dosage | Notes |
| --- | --- | --- | --- |
| Interior cement putty, hand-applied, 1–2 mm | K75 (35,000–40,000) · K100 (45,000–60,000) / EM80 (35,000–45,000) · EM100 (45,000–60,000) | 0.25–0.35 % | Standard putty grades on the TDS; K200 (65,000–80,000) for very absorbent blockwork |
| Exterior cement putty, 2–3 mm | K150 (55,000–65,000) · K200H / EM100H (45,000–60,000) | 0.30–0.40 % | K150: water retention "very high"; EM100H: sag resistance "excellent", heat resistance "excellent" |
| Machine-sprayed skim coat | EM60 (30,000–40,000) · EM80 / K75 | 0.25–0.35 % | Medium viscosity for pumpability; combine with ST2109 or ST3152 starch ether for anti-sag |
| Gypsum finishing putty | ME3570-G (35,000–45,000) · ME4080-G (30,000–40,000) | 0.15–0.30 % | HEMC modified for gypsum: water retention "excellent", final consistency "superior"; K100 / EM100 also list gypsum plasters |
| Ready-mixed (paste) putty | K40HS (20,000–24,000) · K75HS (35,000–40,000) | 0.3–0.5 % | Surface-treated for delayed dissolution and lump-free mixing in water; combine with [Landercoll® HEC](https://landuchina.eu/products-and-solutions/landercoll-cellulose-ether/hec-factory-certified-hydroxyethyl-cellulose-powder/) for storage stability |

**Accurate® redispersible polymer powder**

| Grade family | Grades (TDS Tg / MFFT) | Typical dosage | Use |
| --- | --- | --- | --- |
| Rigid VAE | 5011N, 4012N (Tg 10 ± 5 °C / MFFT 4 °C) | 1–2 % | Interior putty: hardness, no powdering, good sandability — both TDS list wall putty |
| Semi-flexible VAE | 4025N (Tg 0 °C / MFFT 1 °C) | 2–3 % | Exterior putty on render, cement board, AAC |
| Flexible | 5045N (Tg −10 ± 5 °C / MFFT 0 °C), 9055E acrylic–silane (Tg −15 °C) | 3–5 % | Putty over ETICS base coats and substrates with movement; 5045N TDS lists wall putty / skim coat, 9028E/9055E list thermal-insulation putty systems |
| Hydrophobic | 8032H (medium hydrophobic), 8035H (strong hydrophobic), 8048H (very strong, instant-dissolving) | 2–4 % | Wet rooms and façades exposed to driving rain; 8032H and 8035H TDS list skim coat, 8048H lists waterproof putty |

**NOVASTAR® specialty additives**

- Starch ether (HPS), 0.03–0.08 %: ST1506-A (5 % viscosity 500–3,500 mPa·s), ST1506-B (100–800 mPa·s) and ST1403B (300–1,000 mPa·s) are the putty and hand-plaster grades; ST3547 (200–1,500 mPa·s, low ash) and ST3206 (500–2,000 mPa·s) are universal grades for putty, plaster and adhesive mortars. Instant thickening, creamy consistency, less trowel drag, better anti-sag.
- SHP75 / SHP80 silicone hydrophobic powder, 0.2–0.5 % (TDS range 0.1–0.5 %): water-repellent exterior putty, reduced capillary absorption and efflorescence, limited impact on mechanical properties, UV-stable silane/resin active.
- Powder defoamer P805 (standard), P806 (alkali-resistant) or P807 (low-temperature), 0.1–0.2 %: removes pinholes in machine-mixed and sprayed putty.
- Gypsum retarder NOVASTAR® P300 (amino-acid type, TDS dosage 0.05–0.3 % of binder) or P400 / AR-P (modified amino-acid type, TDS dosage 0.001–0.3 %; AR-P alkali-resistant for lime-containing systems): working-time control in gypsum putty; most putties settle between 0.02 and 0.1 %.

Dosages are percentages of the total dry mix for laboratory starting points; the technical data sheets do not prescribe dosages. Confirm with your binder and filler.

Troubleshooting on site

Divider

| Defect | What is happening | Formulation fix |
| --- | --- | --- |
| Powdering / chalking after drying | Water left the layer before the binder hydrated; too little polymer at the surface | Raise cellulose ether by 0.05 % or move to K150 / EM100H; add 1–2 % rigid RDP (5011N); check filler/binder ratio |
| Hairline map cracking | Thick single coat, fast drying, high filler content | Limit coat to ≤ 2 mm per pass; K150 or EM100H for water retention; 2–3 % 4025N; add 0.1 % PP fibre 3 mm for exterior |
| Sagging on walls, slumping in the bucket | Viscosity too low for layer thickness; excess water | EM100H or K200 (sag resistance "excellent"); 0.05 % ST1506-A; reduce water |
| Putty "rolls" or drags under the trowel | Cellulose ether viscosity too high; no starch ether | Step down one viscosity (K200 → K100 → K75); add ST1506-B or ST3547 |
| Hard to sand | Too much RDP or flexible RDP in an interior putty | Reduce to 1–2 % rigid RDP (5011N / 4012N) |
| Pinholes, bubbles | Air entrained during high-speed mixing or spraying | 0.1–0.2 % P805 (P806 in high-alkali cement putty); slower mixer |
| Lumps when mixing paste putty | Standard cellulose ether dissolves on contact and agglomerates | Surface-treated K40HS / K75HS (delayed solubility: "yes" on the TDS) |
| Yellow or dark spots in white putty | Cement or filler impurities, not the additive | Change to white cement / low-iron limestone; cellulose ether and RDP are white to off-white powders |
| Blistering or peeling on exterior putty | Water uptake and freeze; weak bond to render | SHP 0.3 %; hydrophobic RDP 8035H or 8048H; prime absorbent substrate |
| Short working time of gypsum putty | Set not controlled | Gypsum retarder P300 at 0.05 % or P400 at 0.03 %; ME3570-G cellulose ether |

Our field guide [Why wall putty fails on site](https://landuchina.eu/why-wall-putty-fails-on-site/) and the test-based article [Wall putty powdering after drying](https://landuchina.eu/wall-putty-powdering-after-drying-causes-tests-and-formulation-solutions/) go deeper into each case.

HPMC or RDP — which one is missing?

Divider

Formulators often ask whether a powdering putty needs more cellulose ether or more polymer. The quick test: wet the powdered surface. If it re-hardens, the cement never hydrated — add water retention. If it stays soft, the binder is fine but the surface is unbound — add RDP. The full comparison is in [HPMC vs RDP in wall putty](https://landuchina.eu/hpmc-vs-rdp-wall-putty/).

Starting formulations (laboratory basis, dry mix)

Divider

| Component | Interior cement putty | Exterior cement putty | Gypsum finishing putty |
| --- | --- | --- | --- |
| White cement 42.5 | 25–30 % | 30–35 % | — |
| Gypsum hemihydrate | — | — | 60–70 % |
| Limestone / heavy calcium carbonate | 60–70 % | 55–60 % | 25–35 % |
| Light calcium carbonate / talc | 3–5 % | 3–5 % | 3–5 % |
| Landercoll® cellulose ether | K100 0.30 % | EM100H 0.35 % | ME3570-G 0.20 % |
| Accurate® RDP | 5011N 1.5 % | 4025N 2.5 % | 5011N 0.5–1 % |
| NOVASTAR® starch ether | ST1506-B 0.05 % | ST3547 0.05 % | ST1506-A 0.03 % |
| NOVASTAR® SHP75 / SHP80 | — | 0.3 % | — |
| NOVASTAR® gypsum retarder P400 | — | — | 0.02–0.05 % |

These are starting points used in our application laboratory, not finished recipes; raw-material sources and local standards require adjustment and testing.

Products referenced on this page

Divider

- [Landercoll® HPMC for wall putty and skim coat](https://landuchina.eu/products-and-solutions/hpmc-for-wall-putty-skim-coat/) — K75, K100, K150, K200 and the surface-treated K40HS / K75HS, with TDS downloads
- [Landercoll® MHEC for wall putty](https://landuchina.eu/products-and-solutions/mhec-for-wall-putty/) — EM60, EM80, EM100, EM100H, EM200 and the gypsum grades ME3570-G / ME4080-G
- [Accurate® RDP for wall putty](https://landuchina.eu/products-and-solutions/rdp-for-wall-putty/)
- [NOVASTAR® HPS starch ether](https://landuchina.eu/products-and-solutions/hydroxypropyl-starch-ether-hps/) — ST1403B, ST1506-A/B, ST3206, ST3547
- [NOVASTAR® SHP silicone hydrophobic powder](https://landuchina.eu/products-and-solutions/novastar-specialty-additives/novastar-shp-the-ultimate-silicone-hydrophobic-powder-for-building-protection/)
- [NOVASTAR® gypsum retarder](https://landuchina.eu/products-and-solutions/gypsum-retarder/) — P300, P400, AR-P

Working with LANDU

Divider

LANDU has produced cellulose ethers since 2011 and today runs three production bases in Shandong with 75,000 t annual capacity across Landercoll® cellulose ethers, Accurate® RDP and NOVASTAR® additives. The portfolio is REACH-compliant and manufactured under ISO 9001. Putty manufacturers in more than 60 countries use our grades; in Europe we deliver from stock through partners in several countries, including Greece, Spain and Italy. Cellulose ether ships in 25 kg bags on 500 or 600 kg pallets, RDP in 25 kg bags on 600–1,300 kg pallets (neutral or OEM bags available), with a lead time of 7–15 working days for factory shipments.

Skim Coat & Wall Putty Additives: Frequently Asked Questions

Divider

Answers on additive selection, testing, samples and supplier qualification.

How to Change my Photo from Admin Dashboard?

Far far away, behind the word mountains, far from the countries Vokalia and Consonantia, there live the blind texts. Separated they live in Bookmarksgrove right at the coast

Request Samples and a Grade Recommendation

Divider

Tell us the putty type, layer thickness and the defect you are fighting.

We return a grade recommendation and starting dosage within two working days and ship 200–600 g samples free of charge.

REQUEST SAMPLES

**[Ask a Formulation Engineer](https://landuchina.eu/contact-us/)**

*LANDU — Committed to Every Gram.*